BG7

A UV blue bandpass filter that selectively transmits certain wavelength ranges (pass band).

Find more information in the tabs below or on our website.

Use our Interactive Filter Diagram to compare this filter or download our Filter Calculation Tool.

For customized filter products you can mark an article and use the request-button.

*product image is exemplary.

BG7
Spectral values guaranteed
τi (365nm) ≥ 0,25
τi (488nm) ≥ 0,78
τi (633nm) ≤ 0,08
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
Weight
 
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
BG7 - BG7
Thickness
1.0
Reflection factor
0.9185
Internal Transmittance (Table)
λ [nm]
200 < 10⁻³
210 < 10⁻³
220 < 10⁻³
230 < 10⁻³
240 < 10⁻³
250 < 10⁻³
260 < 10⁻³
270 < 10⁻³
280 < 10⁻³
290 < 10⁻³
300 < 10⁻³
310 < 10⁻³
320 < 10⁻³
330 0.013
340 0.066
350 0.160
360 0.260
370 0.349
380 0.435
390 0.504
400 0.561
410 0.614
420 0.657
430 0.695
440 0.728
450 0.754
460 0.776
470 0.788
480 0.794
490 0.788
λ [nm]
500 0.767
510 0.730
520 0.679
530 0.611
540 0.535
550 0.450
560 0.369
570 0.295
580 0.229
590 0.174
600 0.131
610 0.096
620 0.070
630 0.051
640 0.037
650 0.027
660 0.021
670 0.015
680 0.011
690 0.009
700 0.007
710 0.006
720 0.005
730 0.004
740 0.004
750 0.003
760 0.003
770 0.003
780 0.003
790 0.003
λ [nm]
800 0.003
810 0.003
820 0.003
830 0.003
840 0.003
850 0.003
860 0.003
870 0.004
880 0.004
890 0.004
900 0.005
910 0.005
920 0.006
930 0.007
940 0.008
950 0.009
960 0.010
970 0.011
980 0.012
990 0.014
1,000 0.016
1,010 0.018
1,020 0.020
1,030 0.022
1,040 0.024
1,050 0.026
1,060 0.029
1,070 0.033
1,080 0.036
1,090 0.041
λ [nm]
1,100 0.044
1,110 0.048
1,120 0.052
1,130 0.056
1,140 0.062
1,150 0.067
1,160 0.073
1,170 0.078
1,180 0.084
1,190 0.090
1,200 0.096
1,250 0.132
1,300 0.171
1,350 0.215
1,400 0.263
1,450 0.314
1,500 0.363
1,550 0.412
1,600 0.462
1,650 0.508
1,700 0.550
1,750 0.589
1,800 0.624
1,850 0.656
1,900 0.685
1,950 0.712
2,000 0.737
2,050 0.757
2,100 0.774
2,150 0.789
λ [nm]
2,200 0.802
2,250 0.816
2,300 0.827
2,350 0.839
2,400 0.849
2,450 0.860
2,500 0.870
2,550 0.880
2,600 0.887
2,650 0.887
2,700 0.875
2,750 0.767
2,800 0.691
2,850 0.675
2,900 0.672
2,950 0.670
3,000 0.654
3,050 0.628
3,100 0.602
3,150 0.574
3,200 0.546
3,250 0.517
3,300 0.493
3,350 0.471
3,400 0.451
3,450 0.438
3,500 0.433
3,550 0.432
3,600 0.434
3,650 0.438
λ [nm]
3,700 0.444
3,750 0.453
3,800 0.465
3,850 0.478
3,900 0.490
3,950 0.501
4,000 0.503
4,050 0.495
4,100 0.478
4,150 0.456
4,200 0.430
4,250 0.400
4,300 0.366
4,350 0.326
4,400 0.281
4,450 0.230
4,500 0.177
4,550 0.128
4,600 0.090
4,650 0.064
4,700 0.046
4,750 0.036
4,800 0.031
4,850 0.029
4,900 0.027
4,950 0.020
5,000 0.013
5,050 0.006
5,100 0.003
5,150 0.001
Optical values
Reflection factor
Pd 0.918
Reference thickness
d [mm] 1
Spectral values guaranteed
τi (365nm) ≥ 0,25
τi (488nm) ≥ 0,78
τi (633nm) ≤ 0,08
Refractive Indices n
nF (486.1 nm) = 1.526
nh (404.7 nm) = 1.536
ng (435.8 nm) = 1.531
ns (852.1 nm) = 1.511
ne (546.1 nm) = 1.521
nd (587.6 nm) = 1.519
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x 0.262 0.179 0.145
y 0.406 0.360 0.317
Y 30 14 8
λd [nm] 495 492 490
Pe 0.44 0.65 0.76
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x 0.246 0.172 0.143
y 0.382 0.333 0.292
Y 31 16 9
λd [nm] 493 490 488
Pe 0.45 0.66 0.76
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x 0.191 0.152 0.138
y 0.272 0.229 0.200
Y 38 21 13
λd [nm] 486 484 482
Pe 0.49 0.68 0.76
Physical values
Density
p [g/cm3] 2.6028
Bubble content
Bubble class
Transformation temperature
Tg [°C] 447
Temperature coefficient
Tk [nm/°C]
Chemical Resistance
FR class 0
SR class 1.0
AR class 1.0
Thermal expansion
α-30°C/+70°C [10-6/K] 8.7
α20°C/300°C [10-6/K] 10
α20°C/200°C [10-6/K]