S8022

S8022
Spectral values guaranteed
λ (τi, max) [nm] nm nm
λs (τi = 0.00001) [nm] nm
λc (τi = 0.5) [nm] nm nm
Need help or a quote?
CONTACT OUR SUPPORT
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
S8022 - S8022
Thickness
2.0
Reflection factor
0.9099
Internal Transmittance (Table)
λ [nm]
200 < 10⁻³
210 < 10⁻³
220 < 10⁻³
230 < 10⁻³
240 < 10⁻³
250 < 10⁻³
260 < 10⁻³
270 < 10⁻³
280 < 10⁻³
290 < 10⁻³
300 < 10⁻³
310 < 10⁻³
320 < 10⁻³
330 < 10⁻³
340 < 10⁻³
350 < 10⁻³
360 < 10⁻³
370 0.005
380 0.018
390 0.040
400 0.065
410 0.096
420 0.120
430 0.141
440 0.163
450 0.188
460 0.221
470 0.262
480 0.316
490 0.380
λ [nm]
500 0.448
510 0.505
520 0.531
530 0.512
540 0.443
550 0.343
560 0.230
570 0.129
580 0.059
590 0.022
600 0.006
610 0.001
620 < 10⁻³
630 < 10⁻³
640 < 10⁻³
650 < 10⁻³
660 < 10⁻³
670 < 10⁻³
680 < 10⁻³
690 < 10⁻³
700 < 10⁻³
710 < 10⁻³
720 < 10⁻³
730 < 10⁻³
740 < 10⁻³
750 < 10⁻³
760 < 10⁻³
770 < 10⁻³
780 < 10⁻³
790 < 10⁻³
λ [nm]
800 < 10⁻³
810 < 10⁻³
820 < 10⁻³
830 < 10⁻³
840 < 10⁻³
850 < 10⁻³
860 < 10⁻³
870 < 10⁻³
880 < 10⁻³
890 < 10⁻³
900 < 10⁻³
910 < 10⁻³
920 < 10⁻³
930 < 10⁻³
940 < 10⁻³
950 < 10⁻³
960 < 10⁻³
970 < 10⁻³
980 < 10⁻³
990 < 10⁻³
1,000 < 10⁻³
1,010 < 10⁻³
1,020 < 10⁻³
1,030 < 10⁻³
1,040 < 10⁻³
1,050 < 10⁻³
1,060 < 10⁻³
1,070 < 10⁻³
1,080 < 10⁻³
1,090 < 10⁻³
λ [nm]
1,100 < 10⁻³
1,110 < 10⁻³
1,120 < 10⁻³
1,130 < 10⁻³
1,140 < 10⁻³
1,150 < 10⁻³
1,160 < 10⁻³
1,170 < 10⁻³
1,180 < 10⁻³
1,190 < 10⁻³
1,200 < 10⁻³
1,250 < 10⁻³
1,300 < 10⁻³
1,350 < 10⁻³
1,400 < 10⁻³
1,450 < 10⁻³
1,500 < 10⁻³
1,550 < 10⁻³
1,600 < 10⁻³
1,650 0.003
1,700 0.007
1,750 0.016
1,800 0.031
1,850 0.053
1,900 0.083
1,950 0.120
2,000 0.162
2,050 0.207
2,100 0.255
2,150 0.302
λ [nm]
2,200 0.345
2,250 0.387
2,300 0.429
2,350 0.469
2,400 0.506
2,450 0.538
2,500 0.562
2,550 0.577
2,600 0.590
2,650 0.602
2,700 0.606
2,750 0.571
2,800 0.374
2,850 0.213
2,900 0.142
2,950 0.107
3,000 0.086
3,050 0.071
3,100 0.059
3,150 0.050
3,200 0.044
3,250 0.039
3,300 0.037
3,350 0.036
3,400 0.036
3,450 0.037
3,500 0.040
3,550 0.044
3,600 0.049
3,650 0.054
λ [nm]
3,700 0.058
3,750 0.055
3,800 0.044
3,850 0.031
3,900 0.019
3,950 0.009
4,000 0.004
4,050 0.001
4,100 < 10⁻³
4,150 < 10⁻³
4,200 < 10⁻³
4,250 < 10⁻³
4,300 < 10⁻³
4,350 < 10⁻³
4,400 < 10⁻³
4,450 < 10⁻³
4,500 < 10⁻³
4,550 < 10⁻³
4,600 < 10⁻³
4,650 < 10⁻³
4,700 < 10⁻³
4,750 0.001
4,800 0.002
4,850 0.003
4,900 0.003
4,950 0.003
5,000 0.003
5,050 0.002
5,100 0.001
5,150 < 10⁻³
Optical values
Reflection factor
Pd 0.910
Reference thickness
d [mm] 2
Spectral values guaranteed
λ (τi, max) [nm] nm nm
λs (τi = 0.00001) [nm] nm
λc (τi = 0.5) [nm] nm nm
Refractive Indices n
nF (486.1 nm) = 1.564
nh (404.7 nm) = 1.576
ng (435.8 nm) = 1.570
ns (852.1 nm) = 1.549
ne (546.1 nm) = 1.560
nd (587.6 nm) =
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x 0.253 0.203 0.178
y 0.498 0.549 0.593
Y 30 16 9
λd [nm] 503 505 508
Pe 0.44 0.55 0.61
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x 0.241 0.196 0.173
y 0.478 0.530 0.577
Y 31 16 10
λd [nm] 502 504 507
Pe 0.44 0.54 0.60
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x 0.196 0.169 0.154
y 0.374 0.432 0.492
Y 37 21 12
λd [nm] 496 500 505
Pe 0.40 0.47 0.51
Physical values
Density
p [g/cm3] 2.77
Bubble content
Bubble class
Transformation temperature
Tg [°C] 453
Temperature coefficient
Tk [nm/°C]
Chemical Resistance
FR class 0.0
SR class 4.0
AR class 3.0
Thermal expansion
α-30°C/+70°C [10-6/K] 7.8
α20°C/300°C [10-6/K] 8.9
α20°C/200°C [10-6/K]