IRG 24

IRG 24在SWIR,MWIR和LWIR波段具有出色的透射率,并且是IR系列中dn / dT最低的。
低dn / dT和低色散等物理特性,使光学工程师可以设计出没有热散焦效应的颜色校正光学系统。
此外,IRG 24可以通过常规的研磨和抛光,单点金刚石车削或精密模压方式加工,以支持从小批量到大批量的零件制造。
IR characteristics | |
---|---|
成分 | Ge10As40Se50 |
密度 | 4.47 g/cm3 |
热膨胀系数(20°C-100°C) | 20.0·10-6/K |
转变温度 | 225°C |
热变化 dn/dT (1 µm) | 45.9·10-6/K |
热变化 dn/dT (5 µm) | 21.1·10-6/K |
热变化 dn/dT (10 µm) | 20.3·10-6/K |
折射率(10um) | 2.6090 |
表面质量 | 60/40双面抛光 |
表面平整度 | P-V ≤ 5个波长@632.8nm |
倒边 | 安全倒边 |
玻璃类型 |
物品编号 |
直径 |
厚度 |
重量 |
---|

Wavelength [µm] |
Transmission (10 mm) |
Transmission (2 mm) |
Extinction [cm-1] |
---|---|---|---|
0.8 | 52.2 | 87.8 | 0.650 |
1.0 | 91.4 | 98.2 | 0.090 |
1.5 | 96.7 | 99.3 | 0.034 |
2.0 | 97.5 | 99.5 | 0.026 |
2.5 | 97.5 | 99.5 | 0.025 |
3.0 | 98.3 | 99.7 | 0.017 |
3.5 | 98.5 | 99.7 | 0.015 |
4.0 | 98.7 | 99.7 | 0.013 |
4.5 | 96.3 | 99.3 | 0.037 |
5.0 | 97.0 | 99.4 | 0.031 |
5.5 | 99.5 | 99.9 | 0.005 |
6.0 | 99.7 | 99.9 | 0.003 |
6.5 | 99.7 | 99.9 | 0.003 |
7.0 | 99.7 | 99.9 | 0.003 |
7.5 | 99.2 | 99.8 | 0.008 |
8.0 | 95.2 | 99.0 | 0.049 |
Wavelength [µm] |
Transmission (10 mm) |
Transmission (2 mm) |
Extinction [cm-1] |
---|---|---|---|
8.5 | 98.5 | 99.7 | 0.015 |
9.0 | 98.8 | 99.8 | 0.012 |
9.5 | 98.7 | 99.7 | 0.013 |
10.0 | 98.8 | 99.8 | 0.012 |
10.5 | 97.8 | 99.6 | 0.022 |
11.0 | 93.7 | 98.7 | 0.065 |
11.5 | 78.0 | 95.2 | 0.248 |
12.0 | 40.2 | 83.4 | 0.910 |
12.5 | 15.8 | 69.2 | 1.844 |
13.0 | 16.9 | 70.1 | 1.779 |
13.5 | 43.0 | 84.4 | 0.845 |
14.0 | 65.2 | 91.8 | 0.428 |
14.5 | 70.3 | 93.2 | 0.353 |
15.0 | 64.3 | 91.5 | 0.442 |
15.5 | 49.9 | 87.0 | 0.696 |
色散公示常数 | |
---|---|
B1 | 2.8965 |
B2 | 2.9567 |
B3 | 0.9461 |
C1 | 0.0000 |
C2 | 0.1620 |
C3 | 1,939.1000 |
D0 | 1.80·10-5 |
E0 | 2.10·10-5 |
λTK | 1.67·10-3 |
Calculation Formula: Refractive index as a function of wavelength and temperature |
---|
![]() |
Wavelength [µm] |
折射率 (@ 22 °C) |
Δn abs/ΔT [10–6/K] 22 °C |
---|---|---|
0.8 | 2.8028 | 0.0 |
0.9 | 2.7555 | 0.0 |
1.0 | 2.7555 | 46.0 |
1.5 | 2.7249 | 31.3 |
2.0 | 2.6612 | 26.3 |
3.0 | 2.6274 | 22.9 |
4.0 | 2.6222 | 21.7 |
5.0 | 2.6192 | 21.1 |
6.0 | 2.6170 | 20.8 |
7.0 | 2.6151 | 20.6 |
8.0 | 2.6132 | 20.5 |
9.0 | 2.6111 | 20.4 |
10.0 | 2.6090 | 20.3 |
11.0 | 2.6066 | 20.2 |
12.0 | 2.6040 | 20.2 |
Wavelength [µm] |
热变化 [dn/dt] |
---|---|
1 µm | 45.9·10-6/K |
5 µm | 21.1·10-6/K |
10 µm | 20.3·10-6/K |