KG3

玻璃类型 |
物品编号 |
长度 |
宽度 |
厚度 |
重量 |
---|
- SCHOTT
- KG3 - KG3
- 厚度
- 2.0
- 反射系数
- 0.9200
λ [nm] | |
---|---|
200 | |
210 | |
220 | |
230 | |
240 | |
250 | |
260 | < 10⁻³ |
270 | 0.002 |
280 | 0.021 |
290 | 0.087 |
300 | 0.229 |
310 | 0.426 |
320 | 0.618 |
330 | 0.763 |
340 | 0.845 |
350 | 0.895 |
360 | 0.934 |
370 | 0.946 |
380 | 0.951 |
390 | 0.938 |
400 | 0.922 |
410 | 0.908 |
420 | 0.899 |
430 | 0.904 |
440 | 0.911 |
450 | 0.916 |
460 | 0.911 |
470 | 0.917 |
480 | 0.925 |
490 | 0.929 |
λ [nm] | |
---|---|
500 | 0.928 |
510 | 0.926 |
520 | 0.919 |
530 | 0.916 |
540 | 0.920 |
550 | 0.930 |
560 | 0.930 |
570 | 0.927 |
580 | 0.919 |
590 | 0.906 |
600 | 0.890 |
610 | 0.864 |
620 | 0.838 |
630 | 0.805 |
640 | 0.770 |
650 | 0.730 |
660 | 0.689 |
670 | 0.645 |
680 | 0.599 |
690 | 0.550 |
700 | 0.498 |
710 | 0.448 |
720 | 0.399 |
730 | 0.354 |
740 | 0.308 |
750 | 0.265 |
760 | 0.226 |
770 | 0.190 |
780 | 0.158 |
790 | 0.130 |
λ [nm] | |
---|---|
800 | 0.107 |
810 | 0.085 |
820 | 0.069 |
830 | 0.055 |
840 | 0.043 |
850 | 0.034 |
860 | 0.027 |
870 | 0.021 |
880 | 0.016 |
890 | 0.012 |
900 | 0.009 |
910 | 0.007 |
920 | 0.006 |
930 | 0.004 |
940 | 0.003 |
950 | 0.003 |
960 | 0.002 |
970 | 0.002 |
980 | 0.001 |
990 | 0.001 |
1,000 | < 10⁻³ |
1,010 | < 10⁻³ |
1,020 | < 10⁻³ |
1,030 | < 10⁻³ |
1,040 | < 10⁻³ |
1,050 | < 10⁻³ |
1,060 | < 10⁻³ |
1,070 | < 10⁻³ |
1,080 | < 10⁻³ |
1,090 | < 10⁻³ |
λ [nm] | |
---|---|
1,100 | < 10⁻³ |
1,110 | < 10⁻³ |
1,120 | < 10⁻³ |
1,130 | < 10⁻³ |
1,140 | < 10⁻³ |
1,150 | < 10⁻³ |
1,160 | < 10⁻³ |
1,170 | < 10⁻³ |
1,180 | < 10⁻³ |
1,190 | < 10⁻³ |
1,200 | < 10⁻³ |
1,250 | < 10⁻³ |
1,300 | < 10⁻³ |
1,350 | < 10⁻³ |
1,400 | < 10⁻³ |
1,450 | < 10⁻³ |
1,500 | < 10⁻³ |
1,550 | < 10⁻³ |
1,600 | 0.001 |
1,650 | 0.002 |
1,700 | 0.003 |
1,750 | 0.003 |
1,800 | 0.004 |
1,850 | 0.004 |
1,900 | 0.004 |
1,950 | 0.003 |
2,000 | 0.003 |
2,050 | 0.003 |
2,100 | 0.003 |
2,150 | 0.003 |
λ [nm] | |
---|---|
2,200 | 0.003 |
2,250 | 0.003 |
2,300 | 0.004 |
2,350 | 0.004 |
2,400 | 0.006 |
2,450 | 0.007 |
2,500 | 0.009 |
2,550 | 0.012 |
2,600 | 0.014 |
2,650 | 0.017 |
2,700 | 0.019 |
2,750 | 0.014 |
2,800 | 0.002 |
2,850 | < 10⁻³ |
2,900 | < 10⁻³ |
2,950 | < 10⁻³ |
3,000 | < 10⁻³ |
3,050 | < 10⁻³ |
3,100 | < 10⁻³ |
3,150 | < 10⁻³ |
3,200 | < 10⁻³ |
3,250 | < 10⁻³ |
3,300 | < 10⁻³ |
3,350 | < 10⁻³ |
3,400 | < 10⁻³ |
3,450 | < 10⁻³ |
3,500 | < 10⁻³ |
3,550 | < 10⁻³ |
3,600 | 0.001 |
3,650 | 0.002 |
λ [nm] | |
---|---|
3,700 | 0.002 |
3,750 | 0.002 |
3,800 | 0.001 |
3,850 | < 10⁻³ |
3,900 | < 10⁻³ |
3,950 | < 10⁻³ |
4,000 | < 10⁻³ |
4,050 | < 10⁻³ |
4,100 | < 10⁻³ |
4,150 | < 10⁻³ |
4,200 | < 10⁻³ |
4,250 | < 10⁻³ |
4,300 | < 10⁻³ |
4,350 | < 10⁻³ |
4,400 | < 10⁻³ |
4,450 | < 10⁻³ |
4,500 | < 10⁻³ |
4,550 | < 10⁻³ |
4,600 | < 10⁻³ |
4,650 | < 10⁻³ |
4,700 | < 10⁻³ |
4,750 | < 10⁻³ |
4,800 | < 10⁻³ |
4,850 | < 10⁻³ |
4,900 | < 10⁻³ |
4,950 | < 10⁻³ |
5,000 | < 10⁻³ |
5,050 | < 10⁻³ |
5,100 | < 10⁻³ |
5,150 | < 10⁻³ |
反射系数 | |
---|---|
Pd | 0.920 |
参考厚度 | |
---|---|
d [mm] | 2 |
承诺光谱值 | |
---|---|
τi (365nm) | ≥0.86 |
τi (500nm) | ≥0.88 |
τi (600nm) | ≥0.83 |
τi (700nm) | ≤0.55 |
τi (800nm) | ≤0.14 |
τi (900nm) | ≤0.03 |
τi (1060nm) | ≤0.001 |
τi (2200nm) | ≤0.01 |
折射率 n |
---|
nF (486.1 nm) = 1.522 |
nh (404.7 nm) = 1.529 |
ng (435.8 nm) = 1.526 |
ns (852.1 nm) = 1.510 |
ne (546.1 nm) = 1.518 |
nd (587.6 nm) = 1.516 |
色度评估
光源 | A(Planck T = 2347K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.442 | 0.437 | 0.432 |
y | 0.410 | 0.413 | 0.416 |
Y | 86 | 81 | 77 |
λd [nm] | 504 | 505 | 505 |
Pe | 0.01 | 0.02 | 0.04 |
光源 | Planck T = 3200 K | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.418 | 0.413 | 0.409 |
y | 0.401 | 0.404 | 0.406 |
Y | 87 | 82 | 77 |
λd [nm] | 503 | 503 | 503 |
Pe | 0.01 | 0.02 | 0.04 |
光源 | D65 (TC = 6504 K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.309 | 0.306 | 0.303 |
y | 0.330 | 0.332 | 0.333 |
Y | 87 | 82 | 78 |
λd [nm] | 496 | 496 | 496 |
Pe | 0.01 | 0.02 | 0.03 |
密度 | |
---|---|
p [g/cm3] | 2.52 |
气泡含量 | |
---|---|
气泡等级 | 3 |
玻转温度 | |
---|---|
Tg [°C] | 581 |
温度系数 | |
---|---|
Tk [nm/°C] |
耐化学性 | |
---|---|
耐污性 | 0 |
耐酸性 | 2.0 |
耐碱性 | 4.0 |
热膨胀 | |
---|---|
α-30°C/+70°C [10-6/K] | 5.3 |
α20°C/300°C [10-6/K] | 6.1 |
α20°C/200°C [10-6/K] |