S8023

- SCHOTT
- S8023 - S8023
- 厚度
- 3.0
- 反射系数
- 0.9133
λ [nm] | |
---|---|
200 | < 10⁻³ |
210 | < 10⁻³ |
220 | < 10⁻³ |
230 | < 10⁻³ |
240 | < 10⁻³ |
250 | < 10⁻³ |
260 | < 10⁻³ |
270 | < 10⁻³ |
280 | < 10⁻³ |
290 | < 10⁻³ |
300 | < 10⁻³ |
310 | < 10⁻³ |
320 | < 10⁻³ |
330 | < 10⁻³ |
340 | < 10⁻³ |
350 | < 10⁻³ |
360 | 0.012 |
370 | 0.064 |
380 | 0.140 |
390 | 0.210 |
400 | 0.259 |
410 | 0.288 |
420 | 0.304 |
430 | 0.314 |
440 | 0.325 |
450 | 0.343 |
460 | 0.372 |
470 | 0.410 |
480 | 0.461 |
490 | 0.521 |
λ [nm] | |
---|---|
500 | 0.580 |
510 | 0.619 |
520 | 0.622 |
530 | 0.575 |
540 | 0.480 |
550 | 0.353 |
560 | 0.222 |
570 | 0.116 |
580 | 0.049 |
590 | 0.016 |
600 | 0.004 |
610 | < 10⁻³ |
620 | < 10⁻³ |
630 | < 10⁻³ |
640 | < 10⁻³ |
650 | < 10⁻³ |
660 | < 10⁻³ |
670 | < 10⁻³ |
680 | < 10⁻³ |
690 | < 10⁻³ |
700 | < 10⁻³ |
710 | < 10⁻³ |
720 | < 10⁻³ |
730 | < 10⁻³ |
740 | < 10⁻³ |
750 | < 10⁻³ |
760 | < 10⁻³ |
770 | < 10⁻³ |
780 | < 10⁻³ |
790 | < 10⁻³ |
λ [nm] | |
---|---|
800 | < 10⁻³ |
810 | < 10⁻³ |
820 | < 10⁻³ |
830 | < 10⁻³ |
840 | < 10⁻³ |
850 | < 10⁻³ |
860 | < 10⁻³ |
870 | < 10⁻³ |
880 | < 10⁻³ |
890 | < 10⁻³ |
900 | < 10⁻³ |
910 | < 10⁻³ |
920 | < 10⁻³ |
930 | < 10⁻³ |
940 | < 10⁻³ |
950 | < 10⁻³ |
960 | < 10⁻³ |
970 | < 10⁻³ |
980 | < 10⁻³ |
990 | < 10⁻³ |
1,000 | < 10⁻³ |
1,010 | < 10⁻³ |
1,020 | < 10⁻³ |
1,030 | < 10⁻³ |
1,040 | < 10⁻³ |
1,050 | < 10⁻³ |
1,060 | < 10⁻³ |
1,070 | < 10⁻³ |
1,080 | < 10⁻³ |
1,090 | < 10⁻³ |
λ [nm] | |
---|---|
1,100 | < 10⁻³ |
1,110 | < 10⁻³ |
1,120 | < 10⁻³ |
1,130 | < 10⁻³ |
1,140 | < 10⁻³ |
1,150 | < 10⁻³ |
1,160 | < 10⁻³ |
1,170 | < 10⁻³ |
1,180 | < 10⁻³ |
1,190 | < 10⁻³ |
1,200 | < 10⁻³ |
1,250 | < 10⁻³ |
1,300 | < 10⁻³ |
1,350 | < 10⁻³ |
1,400 | < 10⁻³ |
1,450 | < 10⁻³ |
1,500 | < 10⁻³ |
1,550 | < 10⁻³ |
1,600 | < 10⁻³ |
1,650 | 0.001 |
1,700 | 0.004 |
1,750 | 0.011 |
1,800 | 0.024 |
1,850 | 0.044 |
1,900 | 0.072 |
1,950 | 0.107 |
2,000 | 0.149 |
2,050 | 0.195 |
2,100 | 0.243 |
2,150 | 0.291 |
λ [nm] | |
---|---|
2,200 | 0.332 |
2,250 | 0.373 |
2,300 | 0.414 |
2,350 | 0.453 |
2,400 | 0.489 |
2,450 | 0.519 |
2,500 | 0.537 |
2,550 | 0.545 |
2,600 | 0.550 |
2,650 | 0.555 |
2,700 | 0.548 |
2,750 | 0.499 |
2,800 | 0.269 |
2,850 | 0.112 |
2,900 | 0.059 |
2,950 | 0.037 |
3,000 | 0.026 |
3,050 | 0.018 |
3,100 | 0.013 |
3,150 | 0.010 |
3,200 | 0.007 |
3,250 | 0.006 |
3,300 | 0.005 |
3,350 | 0.004 |
3,400 | 0.004 |
3,450 | 0.004 |
3,500 | 0.005 |
3,550 | 0.005 |
3,600 | 0.006 |
3,650 | 0.008 |
λ [nm] | |
---|---|
3,700 | 0.009 |
3,750 | 0.008 |
3,800 | 0.005 |
3,850 | 0.003 |
3,900 | 0.001 |
3,950 | < 10⁻³ |
4,000 | < 10⁻³ |
4,050 | < 10⁻³ |
4,100 | < 10⁻³ |
4,150 | < 10⁻³ |
4,200 | < 10⁻³ |
4,250 | < 10⁻³ |
4,300 | < 10⁻³ |
4,350 | < 10⁻³ |
4,400 | < 10⁻³ |
4,450 | < 10⁻³ |
4,500 | < 10⁻³ |
4,550 | < 10⁻³ |
4,600 | < 10⁻³ |
4,650 | < 10⁻³ |
4,700 | < 10⁻³ |
4,750 | < 10⁻³ |
4,800 | < 10⁻³ |
4,850 | < 10⁻³ |
4,900 | < 10⁻³ |
4,950 | < 10⁻³ |
5,000 | < 10⁻³ |
5,050 | < 10⁻³ |
5,100 | < 10⁻³ |
5,150 | < 10⁻³ |
反射系数 | |
---|---|
Pd | 0.913 |
参考厚度 | |
---|---|
d [mm] | 3 |
折射率 n |
---|
nd (587.6 nm) = |
色度评估
光源 | A(Planck T = 2347K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.277 | 0.218 | 0.189 |
y | 0.459 | 0.474 | 0.486 |
Y | 41 | 27 | 19 |
λd [nm] | 500 | 500 | 500 |
Pe | 0.39 | 0.52 | 0.59 |
光源 | Planck T = 3200 K | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.262 | 0.209 | 0.182 |
y | 0.437 | 0.449 | 0.460 |
Y | 43 | 28 | 21 |
λd [nm] | 498 | 498 | 499 |
Pe | 0.39 | 0.52 | 0.59 |
光源 | D65 (TC = 6504 K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | 0.206 | 0.176 | 0.160 |
y | 0.328 | 0.334 | 0.346 |
Y | 51 | 35 | 26 |
λd [nm] | 491 | 492 | 493 |
Pe | 0.39 | 0.50 | 0.54 |
密度 | |
---|---|
p [g/cm3] | 2.75 |
气泡含量 | |
---|---|
气泡等级 |
玻转温度 | |
---|---|
Tg [°C] | 444 |
温度系数 | |
---|---|
Tk [nm/°C] |
耐化学性 | |
---|---|
耐污性 | 0 |
耐酸性 | 4.0 |
耐碱性 | 3.0 |
热膨胀 | |
---|---|
α-30°C/+70°C [10-6/K] | |
α20°C/300°C [10-6/K] | |
α20°C/200°C [10-6/K] | 9.7 |