NG5

- SCHOTT
- NG5 - NG5
- 厚度
- 1.0
- 反射系数
- 0.9231
λ [nm] | |
---|---|
200 | < 10⁻³ |
210 | < 10⁻³ |
220 | < 10⁻³ |
230 | < 10⁻³ |
240 | < 10⁻³ |
250 | < 10⁻³ |
260 | < 10⁻³ |
270 | < 10⁻³ |
280 | < 10⁻³ |
290 | < 10⁻³ |
300 | < 10⁻³ |
310 | < 10⁻³ |
320 | < 10⁻³ |
330 | 0.016 |
340 | 0.086 |
350 | 0.205 |
360 | 0.328 |
370 | 0.401 |
380 | 0.393 |
390 | 0.500 |
400 | 0.546 |
410 | 0.546 |
420 | 0.549 |
430 | 0.559 |
440 | 0.556 |
450 | 0.569 |
460 | 0.583 |
470 | 0.583 |
480 | 0.577 |
490 | 0.571 |
λ [nm] | |
---|---|
500 | 0.568 |
510 | 0.567 |
520 | 0.568 |
530 | 0.572 |
540 | 0.576 |
550 | 0.577 |
560 | 0.575 |
570 | 0.568 |
580 | 0.561 |
590 | 0.555 |
600 | 0.555 |
610 | 0.558 |
620 | 0.560 |
630 | 0.560 |
640 | 0.558 |
650 | 0.556 |
660 | 0.558 |
670 | 0.564 |
680 | 0.577 |
690 | 0.589 |
700 | 0.599 |
710 | 0.604 |
720 | 0.604 |
730 | 0.600 |
740 | 0.595 |
750 | 0.587 |
760 | 0.580 |
770 | 0.571 |
780 | 0.561 |
790 | 0.551 |
λ [nm] | |
---|---|
800 | 0.542 |
810 | 0.534 |
820 | 0.523 |
830 | 0.514 |
840 | 0.505 |
850 | 0.495 |
860 | 0.486 |
870 | 0.480 |
880 | 0.473 |
890 | 0.464 |
900 | 0.458 |
910 | 0.449 |
920 | 0.442 |
930 | 0.436 |
940 | 0.429 |
950 | 0.422 |
960 | 0.417 |
970 | 0.410 |
980 | 0.405 |
990 | 0.402 |
1,000 | 0.397 |
1,010 | 0.394 |
1,020 | 0.390 |
1,030 | 0.387 |
1,040 | 0.385 |
1,050 | 0.383 |
1,060 | 0.380 |
1,070 | 0.379 |
1,080 | 0.377 |
1,090 | 0.376 |
λ [nm] | |
---|---|
1,100 | 0.379 |
1,110 | 0.381 |
1,120 | 0.381 |
1,130 | 0.382 |
1,140 | 0.382 |
1,150 | 0.383 |
1,160 | 0.383 |
1,170 | 0.384 |
1,180 | 0.386 |
1,190 | 0.388 |
1,200 | 0.390 |
1,250 | 0.407 |
1,300 | 0.440 |
1,350 | 0.468 |
1,400 | 0.500 |
1,450 | 0.532 |
1,500 | 0.560 |
1,550 | 0.576 |
1,600 | 0.586 |
1,650 | 0.590 |
1,700 | 0.590 |
1,750 | 0.593 |
1,800 | 0.595 |
1,850 | 0.600 |
1,900 | 0.610 |
1,950 | 0.619 |
2,000 | 0.630 |
2,050 | 0.641 |
2,100 | 0.650 |
2,150 | 0.657 |
λ [nm] | |
---|---|
2,200 | 0.662 |
2,250 | 0.671 |
2,300 | 0.680 |
2,350 | 0.688 |
2,400 | 0.690 |
2,450 | 0.695 |
2,500 | 0.700 |
2,550 | 0.702 |
2,600 | 0.704 |
2,650 | 0.700 |
2,700 | 0.660 |
2,750 | 0.311 |
2,800 | 0.170 |
2,850 | 0.158 |
2,900 | 0.170 |
2,950 | 0.194 |
3,000 | 0.220 |
3,050 | 0.248 |
3,100 | 0.280 |
3,150 | 0.306 |
3,200 | 0.336 |
3,250 | 0.363 |
3,300 | 0.370 |
3,350 | 0.351 |
3,400 | 0.290 |
3,450 | 0.217 |
3,500 | 0.150 |
3,550 | 0.101 |
3,600 | 0.070 |
3,650 | 0.059 |
λ [nm] | |
---|---|
3,700 | 0.071 |
3,750 | 0.108 |
3,800 | 0.140 |
3,850 | 0.158 |
3,900 | 0.147 |
3,950 | 0.118 |
4,000 | 0.100 |
4,050 | 0.089 |
4,100 | 0.095 |
4,150 | 0.100 |
4,200 | 0.100 |
4,250 | 0.094 |
4,300 | 0.078 |
4,350 | 0.055 |
4,400 | 0.040 |
4,450 | 0.025 |
4,500 | 0.016 |
4,550 | 0.010 |
4,600 | 0.006 |
4,650 | 0.003 |
4,700 | 0.002 |
4,750 | 0.001 |
4,800 | < 10⁻³ |
4,850 | < 10⁻³ |
4,900 | < 10⁻³ |
4,950 | < 10⁻³ |
5,000 | < 10⁻³ |
5,050 | < 10⁻³ |
5,100 | < 10⁻³ |
5,150 | < 10⁻³ |
反射系数 | |
---|---|
Pd | 0.923 |
参考厚度 | |
---|---|
d [mm] | 1 |
承诺光谱值 | |
---|---|
τi (405nm) | =0.56± 0,03 |
τi (546nm) | =0.57± 0,03 |
τi (694nm) | =0.62± 0,03 |
折射率 n |
---|
nd (587.6 nm) = 1.500 |
色度评估
光源 | A(Planck T = 2347K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
光源 | Planck T = 3200 K | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
光源 | D65 (TC = 6504 K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
密度 | |
---|---|
p [g/cm3] | 2.43 |
气泡含量 | |
---|---|
气泡等级 | 2 |
玻转温度 | |
---|---|
Tg [°C] | 474 |
温度系数 | |
---|---|
Tk [nm/°C] |
耐化学性 | |
---|---|
耐污性 | 1 |
耐酸性 | 3.2 |
耐碱性 | 2.0 |
热膨胀 | |
---|---|
α-30°C/+70°C [10-6/K] | 6.6 |
α20°C/300°C [10-6/K] | 7.3 |
α20°C/200°C [10-6/K] |