RG830

- SCHOTT
- RG830 - RG830
- 厚度
- 3.0
- 反射系数
- 0.9087
λ [nm] | |
---|---|
200 | < 10⁻³ |
210 | < 10⁻³ |
220 | < 10⁻³ |
230 | < 10⁻³ |
240 | < 10⁻³ |
250 | < 10⁻³ |
260 | < 10⁻³ |
270 | < 10⁻³ |
280 | < 10⁻³ |
290 | < 10⁻³ |
300 | < 10⁻³ |
310 | < 10⁻³ |
320 | < 10⁻³ |
330 | < 10⁻³ |
340 | < 10⁻³ |
350 | < 10⁻³ |
360 | < 10⁻³ |
370 | < 10⁻³ |
380 | < 10⁻³ |
390 | < 10⁻³ |
400 | < 10⁻³ |
410 | < 10⁻³ |
420 | < 10⁻³ |
430 | < 10⁻³ |
440 | < 10⁻³ |
450 | < 10⁻³ |
460 | < 10⁻³ |
470 | < 10⁻³ |
480 | < 10⁻³ |
490 | < 10⁻³ |
λ [nm] | |
---|---|
500 | < 10⁻³ |
510 | < 10⁻³ |
520 | < 10⁻³ |
530 | < 10⁻³ |
540 | < 10⁻³ |
550 | < 10⁻³ |
560 | < 10⁻³ |
570 | < 10⁻³ |
580 | < 10⁻³ |
590 | < 10⁻³ |
600 | < 10⁻³ |
610 | < 10⁻³ |
620 | < 10⁻³ |
630 | < 10⁻³ |
640 | < 10⁻³ |
650 | < 10⁻³ |
660 | < 10⁻³ |
670 | < 10⁻³ |
680 | < 10⁻³ |
690 | < 10⁻³ |
700 | < 10⁻³ |
710 | < 10⁻³ |
720 | < 10⁻³ |
730 | < 10⁻³ |
740 | < 10⁻³ |
750 | < 10⁻³ |
760 | < 10⁻³ |
770 | < 10⁻³ |
780 | 0.002 |
790 | 0.008 |
λ [nm] | |
---|---|
800 | 0.030 |
810 | 0.099 |
820 | 0.260 |
830 | 0.490 |
840 | 0.699 |
850 | 0.837 |
860 | 0.919 |
870 | 0.958 |
880 | 0.977 |
890 | 0.985 |
900 | 0.990 |
910 | 0.993 |
920 | 0.994 |
930 | 0.995 |
940 | 0.995 |
950 | 0.996 |
960 | 0.996 |
970 | 0.996 |
980 | 0.996 |
990 | 0.996 |
1,000 | 0.996 |
1,010 | 0.996 |
1,020 | 0.996 |
1,030 | 0.996 |
1,040 | 0.997 |
1,050 | 0.997 |
1,060 | 0.997 |
1,070 | 0.997 |
1,080 | 0.997 |
1,090 | 0.997 |
λ [nm] | |
---|---|
1,100 | 0.997 |
1,110 | 0.997 |
1,120 | 0.997 |
1,130 | 0.997 |
1,140 | 0.997 |
1,150 | 0.997 |
1,160 | 0.997 |
1,170 | 0.998 |
1,180 | 0.998 |
1,190 | 0.998 |
1,200 | 0.998 |
1,250 | 0.998 |
1,300 | 0.999 |
1,350 | 1.000 |
1,400 | 0.998 |
1,450 | 0.999 |
1,500 | 1.000 |
1,550 | 1.000 |
1,600 | 1.000 |
1,650 | 0.998 |
1,700 | 0.996 |
1,750 | 0.994 |
1,800 | 0.992 |
1,850 | 0.991 |
1,900 | 0.990 |
1,950 | 0.989 |
2,000 | 0.987 |
2,050 | 0.985 |
2,100 | 0.983 |
2,150 | 0.976 |
λ [nm] | |
---|---|
2,200 | 0.966 |
2,250 | 0.955 |
2,300 | 0.956 |
2,350 | 0.953 |
2,400 | 0.946 |
2,450 | 0.939 |
2,500 | 0.936 |
2,550 | 0.933 |
2,600 | 0.923 |
2,650 | 0.904 |
2,700 | 0.865 |
2,750 | 0.500 |
2,800 | 0.218 |
2,850 | 0.166 |
2,900 | 0.137 |
2,950 | 0.117 |
3,000 | 0.100 |
3,050 | 0.086 |
3,100 | 0.077 |
3,150 | 0.070 |
3,200 | 0.066 |
3,250 | 0.063 |
3,300 | 0.059 |
3,350 | 0.056 |
3,400 | 0.052 |
3,450 | 0.049 |
3,500 | 0.046 |
3,550 | 0.043 |
3,600 | 0.044 |
3,650 | 0.045 |
λ [nm] | |
---|---|
3,700 | 0.041 |
3,750 | 0.036 |
3,800 | 0.034 |
3,850 | 0.041 |
3,900 | 0.051 |
3,950 | 0.066 |
4,000 | 0.067 |
4,050 | 0.059 |
4,100 | 0.051 |
4,150 | 0.048 |
4,200 | 0.054 |
4,250 | 0.056 |
4,300 | 0.051 |
4,350 | 0.043 |
4,400 | 0.033 |
4,450 | 0.022 |
4,500 | 0.013 |
4,550 | 0.007 |
4,600 | 0.003 |
4,650 | 0.001 |
4,700 | < 10⁻³ |
4,750 | < 10⁻³ |
4,800 | < 10⁻³ |
4,850 | < 10⁻³ |
4,900 | < 10⁻³ |
4,950 | < 10⁻³ |
5,000 | < 10⁻³ |
5,050 | < 10⁻³ |
5,100 | < 10⁻³ |
5,150 | < 10⁻³ |
反射系数 | |
---|---|
Pd | 0.909 |
参考厚度 | |
---|---|
d [mm] | 3 |
承诺光谱值 | |
---|---|
λs (τi = 0.00001) [nm] | 670 |
λc (τi = 0.5) [nm] | 830 ± 9 |
λp1 (τi = 0.92) [nm] | 950 |
折射率 n |
---|
ns (852.1 nm) = 1.550 |
nd (587.6 nm) = 1.560 |
色度评估
光源 | A(Planck T = 2347K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
光源 | Planck T = 3200 K | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
光源 | D65 (TC = 6504 K) | ||
---|---|---|---|
d [mm] | 1 | 2 | 3 |
x | |||
y | |||
Y | |||
λd [nm] | |||
Pe |
密度 | |
---|---|
p [g/cm3] | 2.94 |
气泡含量 | |
---|---|
气泡等级 | 3 |
玻转温度 | |
---|---|
Tg [°C] | 554 |
温度系数 | |
---|---|
Tk [nm/°C] | 0.23 |
耐化学性 | |
---|---|
耐污性 | 5 |
耐酸性 | 53.4 |
耐碱性 | 1.3 |
热膨胀 | |
---|---|
α-30°C/+70°C [10-6/K] | 9.5 |
α20°C/300°C [10-6/K] | 10.5 |
α20°C/200°C [10-6/K] |