Spectral values guaranteed
λs (τi = 0.00001) [nm] 730 nm
λc (τi = 0.5) [nm] 1000 nm ± 6 nm
λp1 (τi = 0.9) [nm] 1300 nm
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
Weight
 
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
RG1000 - RG1000
Thickness
3.0
Reflection factor
0.9133
Internal Transmittance (Table)
λ [nm]
200 < 10⁻³
210 < 10⁻³
220 < 10⁻³
230 < 10⁻³
240 < 10⁻³
250 < 10⁻³
260 < 10⁻³
270 < 10⁻³
280 < 10⁻³
290 < 10⁻³
300 < 10⁻³
310 < 10⁻³
320 < 10⁻³
330 < 10⁻³
340 < 10⁻³
350 < 10⁻³
360 < 10⁻³
370 < 10⁻³
380 < 10⁻³
390 < 10⁻³
400 < 10⁻³
410 < 10⁻³
420 < 10⁻³
430 < 10⁻³
440 < 10⁻³
450 < 10⁻³
460 < 10⁻³
470 < 10⁻³
480 < 10⁻³
490 < 10⁻³
λ [nm]
500 < 10⁻³
510 < 10⁻³
520 < 10⁻³
530 < 10⁻³
540 < 10⁻³
550 < 10⁻³
560 < 10⁻³
570 < 10⁻³
580 < 10⁻³
590 < 10⁻³
600 < 10⁻³
610 < 10⁻³
620 < 10⁻³
630 < 10⁻³
640 < 10⁻³
650 < 10⁻³
660 < 10⁻³
670 < 10⁻³
680 < 10⁻³
690 < 10⁻³
700 < 10⁻³
710 < 10⁻³
720 < 10⁻³
730 < 10⁻³
740 < 10⁻³
750 < 10⁻³
760 < 10⁻³
770 < 10⁻³
780 < 10⁻³
790 < 10⁻³
λ [nm]
800 < 10⁻³
810 < 10⁻³
820 < 10⁻³
830 0.002
840 0.003
850 0.007
860 0.013
870 0.022
880 0.036
890 0.052
900 0.077
910 0.107
920 0.141
930 0.182
940 0.225
950 0.273
960 0.318
970 0.368
980 0.413
990 0.461
1,000 0.503
1,010 0.546
1,020 0.585
1,030 0.619
1,040 0.653
1,050 0.682
1,060 0.708
1,070 0.732
1,080 0.754
1,090 0.773
λ [nm]
1,100 0.792
1,110 0.808
1,120 0.823
1,130 0.835
1,140 0.846
1,150 0.856
1,160 0.866
1,170 0.874
1,180 0.882
1,190 0.888
1,200 0.894
1,250 0.918
1,300 0.934
1,350 0.944
1,400 0.952
1,450 0.958
1,500 0.964
1,550 0.969
1,600 0.972
1,650 0.975
1,700 0.976
1,750 0.977
1,800 0.976
1,850 0.975
1,900 0.973
1,950 0.971
2,000 0.969
2,050 0.966
2,100 0.962
2,150 0.955
λ [nm]
2,200 0.944
2,250 0.934
2,300 0.932
2,350 0.928
2,400 0.922
2,450 0.914
2,500 0.905
2,550 0.896
2,600 0.886
2,650 0.874
2,700 0.837
2,750 0.572
2,800 0.446
2,850 0.424
2,900 0.414
2,950 0.394
3,000 0.370
3,050 0.337
3,100 0.301
3,150 0.264
3,200 0.230
3,250 0.201
3,300 0.175
3,350 0.151
3,400 0.130
3,450 0.117
3,500 0.109
3,550 0.103
3,600 0.099
3,650 0.098
λ [nm]
3,700 0.098
3,750 0.100
3,800 0.104
3,850 0.108
3,900 0.114
3,950 0.118
4,000 0.116
4,050 0.109
4,100 0.098
4,150 0.086
4,200 0.072
4,250 0.059
4,300 0.043
4,350 0.029
4,400 0.018
4,450 0.009
4,500 0.003
4,550 0.001
4,600 < 10⁻³
4,650 < 10⁻³
4,700 < 10⁻³
4,750 < 10⁻³
4,800 < 10⁻³
4,850 < 10⁻³
4,900 < 10⁻³
4,950 < 10⁻³
5,000 < 10⁻³
5,050 < 10⁻³
5,100 < 10⁻³
5,150 < 10⁻³
Optical values
Reflection factor
Pd 0.913
Reference thickness
d [mm] 3
Spectral values guaranteed
λs (τi = 0.00001) [nm] 730 nm
λc (τi = 0.5) [nm] 1000 nm ± 6 nm
λp1 (τi = 0.9) [nm] 1300 nm
Refractive Indices n
nF (486.1 nm) = 1.548
nh (404.7 nm) = 1.558
ng (435.8 nm) = 1.554
ns (852.1 nm) = 1.532
ne (546.1 nm) = 1.543
nd (587.6 nm) = 1.541
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Physical values
Density
p [g/cm3] 2.73
Bubble content
Bubble class 3
Transformation temperature
Tg [°C] 476
Temperature coefficient
Tk [nm/°C] 0.41
Chemical Resistance
FR class 0
SR class 1.0
AR class 1.0
Thermal expansion
α-30°C/+70°C [10-6/K] 9
α20°C/300°C [10-6/K] 10.23
α20°C/200°C [10-6/K]