UG1

A bandpass filter that shows its highest transmission in the UV wavelength ranges (pass band).

Find more information in the tabs below or on our website.

Use our Interactive Filter Diagram to compare this filter or download our Filter Calculation Tool.

For customized filter products you can mark an article and use the request-button.

*product image is exemplary.

UG1
Spectral values guaranteed
τi (365nm) ≥ 0,8
τi (405nm) ≤ 0,1
τi (694nm) ≤ 0,06
τi (750nm) ≤ 0,53
Sign in to choose your product

As a registered user in our shop you enjoy many advantages

  • Simply order
  • Stock overview
  • Simple profile management
Need help or a quote?
CONTACT OUR SUPPORT
Article Details
SCHOTT
Article
Glass type
L
W
T
Weight
 
Technical Details
Internal Transmittance (Chart)

Only values between 0.1 and 30 with one decimal place are allowed.

SCHOTT
UG1 - UG1
Thickness
1.0
Reflection factor
0.9132
Internal Transmittance (Table)
λ [nm]
200
210
220
230
240
250
260 < 10⁻³
270 < 10⁻³
280 0.002
290 0.037
300 0.155
310 0.335
320 0.519
330 0.659
340 0.751
350 0.807
360 0.833
370 0.812
380 0.706
390 0.438
400 0.138
410 0.017
420 < 10⁻³
430 < 10⁻³
440 < 10⁻³
450 < 10⁻³
460 < 10⁻³
470 < 10⁻³
480 < 10⁻³
490 < 10⁻³
λ [nm]
500 < 10⁻³
510 < 10⁻³
520 < 10⁻³
530 < 10⁻³
540 < 10⁻³
550 < 10⁻³
560 < 10⁻³
570 < 10⁻³
580 < 10⁻³
590 < 10⁻³
600 < 10⁻³
610 < 10⁻³
620 < 10⁻³
630 < 10⁻³
640 < 10⁻³
650 < 10⁻³
660 < 10⁻³
670 < 10⁻³
680 < 10⁻³
690 0.002
700 0.028
710 0.139
720 0.269
730 0.368
740 0.450
750 0.480
760 0.442
770 0.374
780 0.330
790 0.307
λ [nm]
800 0.277
810 0.242
820 0.209
830 0.181
840 0.158
850 0.140
860 0.125
870 0.112
880 0.102
890 0.093
900 0.087
910 0.081
920 0.076
930 0.073
940 0.069
950 0.066
960 0.065
970 0.063
980 0.063
990 0.061
1,000 0.060
1,010 0.059
1,020 0.057
1,030 0.056
1,040 0.053
1,050 0.051
1,060 0.049
1,070 0.047
1,080 0.045
1,090 0.042
λ [nm]
1,100 0.039
1,110 0.037
1,120 0.035
1,130 0.033
1,140 0.030
1,150 0.029
1,160 0.027
1,170 0.026
1,180 0.024
1,190 0.023
1,200 0.022
1,250 0.020
1,300 0.021
1,350 0.025
1,400 0.026
1,450 0.024
1,500 0.023
1,550 0.025
1,600 0.027
1,650 0.027
1,700 0.021
1,750 0.018
1,800 0.017
1,850 0.018
1,900 0.021
1,950 0.025
2,000 0.030
2,050 0.035
2,100 0.042
2,150 0.050
λ [nm]
2,200 0.060
2,250 0.072
2,300 0.083
2,350 0.096
2,400 0.108
2,450 0.120
2,500 0.126
2,550 0.152
2,600 0.162
2,650 0.170
2,700 0.176
2,750 0.150
2,800 0.120
2,850 0.122
2,900 0.128
2,950 0.135
3,000 0.140
3,050 0.144
3,100 0.148
3,150 0.151
3,200 0.155
3,250 0.158
3,300 0.162
3,350 0.167
3,400 0.172
3,450 0.177
3,500 0.182
3,550 0.189
3,600 0.200
3,650 0.207
λ [nm]
3,700 0.215
3,750 0.223
3,800 0.240
3,850 0.259
3,900 0.277
3,950 0.286
4,000 0.289
4,050 0.291
4,100 0.292
4,150 0.293
4,200 0.293
4,250 0.289
4,300 0.276
4,350 0.252
4,400 0.220
4,450 0.186
4,500 0.150
4,550 0.113
4,600 0.080
4,650 0.055
4,700 0.040
4,750 0.028
4,800 0.020
4,850 0.014
4,900 0.011
4,950 0.008
5,000 0.006
5,050 0.004
5,100 0.002
5,150 0.001
Optical values
Reflection factor
Pd 0.913
Reference thickness
d [mm] 1
Spectral values guaranteed
τi (365nm) ≥ 0,8
τi (405nm) ≤ 0,1
τi (694nm) ≤ 0,06
τi (750nm) ≤ 0,53
Refractive Indices n
nF (486.1 nm) = 1.548
nh (404.7 nm) = 1.557
ng (435.8 nm) = 1.553
ns (852.1 nm) = 1.533
ne (546.1 nm) = 1.543
nd (587.6 nm) = 1.541
Colorimetric evaluation
Illuminant A(Planck T = 2347K)
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Illuminant Planck T = 3200 K
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Illuminant D65 (TC = 6504 K)
d [mm] 1 2 3
x
y
Y
λd [nm]
Pe
Physical values
Density
p [g/cm3] 2.7791
Bubble content
Bubble class
Transformation temperature
Tg [°C] 580
Temperature coefficient
Tk [nm/°C]
Chemical Resistance
FR class 0
SR class 1.0
AR class 1.0
Thermal expansion
α-30°C/+70°C [10-6/K] 7.9
α20°C/300°C [10-6/K] 8.97
α20°C/200°C [10-6/K]